Extract

The infiltration of porous and particulate materials for metallographic examination with low-melting alloys was first described by Rose and DeRoos . The use of Wood's metal to fill porosity in sandstone was reported by Craze , by Dullien , and by Yadev et al. . Changes in pore structure and phase dispersions in iron ore pellets after simulated blast furnace reduction were reported by Shultz et al. , wherein liquid Bi-Sn impregnation was used to prepare cross sections of deformed and reduced pellets for backscatter electron imaging. Steele and Engel also applied the technique to examine the microstructure in commercial boron nitride (BN). In that study porosity formed by leaching the B2O3 phase was filled with liquid metal to allow argon-ion etching to expose the BN microstructure. The characterization of cracks and porosity in cement-based materials after filling with Wood's metal has been reported by Nemati et al. . Cracks developed during compression testing of marble were studied by in-situ metal impregnation in Chang et al. .

Type
Instrumentation
Copyright
Copyright © Microscopy Society of America 2010

Introduction

The infiltration of porous and particulate materials for metallographic examination with low-melting alloys was first described by Rose and DeRoos [Reference Rose, DeRoos, Gray and McCall1]. The use of Wood's metal to fill porosity in sandstone was reported by Craze [Reference Craze2], by Dullien [Reference Dullien3], and by Yadev et al. [Reference Yadev, Dullian, Chatzis and Macdonald4]. Changes in pore structure and phase dispersions in iron ore pellets after simulated blast furnace reduction were reported by Shultz et al. [Reference Shultz, Lyons and Steele5], wherein liquid Bi-Sn impregnation was used to prepare cross sections of deformed and reduced pellets for backscatter electron imaging. Steele and Engel [Reference Steele and Engel6] also applied the technique to examine the microstructure in commercial boron nitride (BN). In that study porosity formed by leaching the B2O3 phase was filled with liquid metal to allow argon-ion etching to expose the BN microstructure. The characterization of cracks and porosity in cement-based materials after filling with Wood's metal has been reported by Nemati et al. [Reference Nemati, Monteiro and Scrivener7, Reference Scrivener and Nemati8]. Cracks developed during compression testing of marble were studied by in-situ metal impregnation in Chang et al. [Reference Chang, Monteiro, Nemati and Shyu9].

The technique, which will be described in this article, involves pressure impregnation with low-melting liquid bismuth (Bi) alloys that shrink or have a low-volume expansion when they solidify. This leads to penetration of open pores according to the classic mercury intrusion relation when the liquid alloy is non-wetting for the material being impregnated (Ritter and Drake) [Reference Ritter and Drake10]. The diameter of the smallest pore opening penetrated by the liquid metal is given by:

(1)

In this equation, p is the pressure on the liquid, θ is the contact angle between the liquid and solid being impregnated, and σ is the surface tension of the liquid alloy. If the contact angle θ ∼ 140° and the surface tension σ ∼ 480 dynes/cm (as for mercury with a ceramic material), then d = 213/p, where d is in µm when p is in psi. Thus at p = 5,000 psi the smallest pore that would be penetrated by the liquid metal would be, d = 0.04 µm (400 Å), and at p = 10,000 psi then d = 0.02 µm. Hence porous materials and powders with extremely small open porosity can be filled by pressure impregnation with a low-melting liquid alloy and prepared for examination by standard grinding and polishing methods. This infiltration technique is essentially the same as a Mercury Porosimetry experiment of Ritter and Drake [Reference Ritter and Drake10] with a slightly higher temperature.

Some of the advantages obtained using this mounting technique include grinding and polishing of friable materials without pull-outs or damage to the porous material, characterization using electron probe instruments of many materials without coating, and the ability to argon-ion etch the mechanically polished samples. These advantages will be illustrated by several specific examples of porous materials that are difficult to prepare and examine with an SEM or microprobe.

The Pressure Impregnation Technique

Several commercial alloys that can be used for the impregnation of porous samples and powders are listed with their properties in Appendix 1. These alloys include Bi as the major alloying element, because it produces low-melting eutectic type alloys, and has the unusual property of expanding upon solidification. The most effective alloy, because of its hardness and solidification properties, is Cerrotru™ (58wt%Bi and 42wt%Sn), which solidifies at or below the eutectic temperature of 138°C. Lower melting point alloys, including CerroBend™, which has its eutectic melting temperature at ∼70°C, and Indalloy™, which melts at ∼ 47°C, can be used if the porous material is sensitive to or changed by the 150°C heating required for Cerrotru™.

The pressure impregnation experiment can be carried out in a standard mounting press if O-rings are used for containment of the liquid alloy under pressure. Two O-ring holders must be machined to allow an O-ring seal against both the top and bottom pistons of the mounting press when pressure is applied. Figure 1 shows a schematic diagram of this type of pressure chamber.

Figure 1. Diagram showing the mounting press with O-rings hold the liquid metal under the pressure needed to infiltrate a porous sample.

Heating the mounting cylinder to above the liquidus temperature for the alloy being used and then increasing the pressure will cause the non-wetting liquid metal to penetrate all open-pore throats larger than diameter d, (as given by the Washburn equation 1). Thus by applying 10 ksi pressure, all open-pore throats larger than about 20 mm (200 Å) will be penetrated and open porosity will be filled with the liquid metal. Cooling the cylinder to solidify the liquid metal while maintaining the pressure will produce a metallographic mount that can be ground and polished by standard methods. Figure 2 shows a macro-photograph of a 1-inch diameter Cerrotru™ mount of a sample of a partially reduced hematite pellet as described in Shultz et al. [Reference Shultz, Lyons and Steele5].

Figure 2. Photograph of a 1-inch diameter Cerrotru alloy mount of a partially reduced Taconite (Hematite) pellet from Shultz et al. [Reference Shultz, Lyons and Steele5].

Results

In the following examples, SEM micro-graphs of porous materials and powder samples that have been mounted using the pressure-impregnation technique will be presented and discussed. These include images of the following microstructures: (1) mono-size (0.5 micron) silica sphere packing, (2) New Mexican ancient pueblo pottery, (3) magnesia refractory brick, and (4) wood (dried cedar).

Example 1: Micrographs from a 0.5 Micron Mono-size Silica Sphere Packing

Mono-size silica sphere packings with diameters of 0.2 to 0.5 microns are similar in structure to natural or synthetic opals [Reference Xia, Gates, Yin and Lu11]. Figure 3 shows a secondary electron image from a fracture surface of 425-nm diameter spheres packed in a regular array [Reference Mayoral, Requena, Lopez, Moya, Miguez, Vazquez, Meseguer, Holgado, Cintas and Blanco12], which shows both ⟨100⟩ and ⟨111⟩ type planes. Figures 4 and 5 show backscattered electron images of cross sections prepared after liquid metal impregnation of a lightly sintered packing of 0.5-µm diameter mono-size silica spheres.

Figure 3. Fracture surface of 425-nm mono-size silica sphere packing showing 100 type planes and close-packed 111-type planes (from Mayoral et al. [Reference Mayoral, Requena, Lopez, Moya, Miguez, Vazquez, Meseguer, Holgado, Cintas and Blanco12]).

Figure 4. Backscatter image of 0.5 micron silica sphere packing that has been filled with Bi-Sn alloy. The stacking faults and the grain-like packing of the spherical particles can be observed.

Figure 5. A higher magnification BSE image of a polished section of 0.5 micron silica sphere packing showing filled interstices through the silica particles.

Example 2: Microstructure of Ancient Pueblo Pottery

The microstructure of pottery shards from an Anazazi pueblo ruin in New Mexico [Reference Steele13] were examined after filling with liquid Cerrotru™ and mechanically polishing. The sections were examined using backscatter imaging in an SEM. Figures 6 and 7 are inverted backscatter images that show prior porosity (now filled with Bi-Sn alloy) as dark contrast and clay and temper particles with lighter contrast. The micrographs were obtained without coating. Figure 7 shows the clay microstructure, which has been suggested to be partially transformed to mullite.

Figure 6. Inverted BS image of pottery shard after filling with Bi-Sn and polishing. Varying gray shades are the result of atomic number contrast.

Figure 7. Higher magnification view of the microstructure of a pottery shard. Note that the clay microstructure consists of two phases that may be the result of incomplete transformation to mullite.

Example 3: Magnesia-Chromite Refractory Brick

The microstructure of magnesia (MgO)-chromite (Cr2O3) refractory brick [Reference Steele14] is illustrated with the inverted backscatter electron micrographs (shown in Figures 8, 9, 10, and 11). Open porosity is filled with liquid Bi-Sn allowing argon-ion etching to be used to expose fine spinel precipitates within the MgO. These spinel precipitates form as a result of diffusion of Cr or Fe from the chromite or hematite ore particles (Ostyn) [Reference Ostyn, Carter, Koehne, Falke and Schmalzried15] where they are bonded to the MgO. Figure 8 gives a low-magnification inverted backscatter image of the MgO refractory brick, where the Bi-Sn filled pores and cracks are black and the MgO is white. Chromite and hematite ore particles, which are used as initial constituents in the brick, are shown by atomic number contrast with varying shades of gray.

Figure 8. Low-magnification inverted backscatter image of a magnesia-chromite refractory brick. Note: MgO = white, Pores (P) = black, Cr2O3 = light gray, and Fe2O3 = dark gray.

Figure 9. Inverted backscatter image showing chromite interface and spinel precipitates within the MgO phase. The filled pores and cracks that connect them can be readily observed. The scale marker is 0.1 mm.

Figure 10. Higher-magnification backscatter image of MgO regions showing SiO2 layers separating MgO grains that have fine spinel precipitates formed within them.

Figure 11. High-magnification inverted backscatter image showing a silica layer between MgO grains that contain fine spinel precipitates. Argon-ion etching of the mechanically polished surface is required to observe these fine cruciform-shaped spinel precipitates.

Example 4: Microstructure of Dried Cedar

Figures 12 and 13 show the microstructure of dried cedar in inverted backscatter images. The dark regions are pores that were filled in by the Bi-Sn impregnation. The low-magnification image shown in Figure 12 shows the ring pattern and the different types of cells formed by the tree. The higher-magnification image (Figure 13) shows the fine micro-cracks present in the dried wood and the different types of cells present in cedar. The larger cells are likely vessels, and the double cells separated by a thin wall are likely tracheids (illustrated in Figure 13) in the cedar structure. The cracking pattern in the walls of the fine wood fibers is clearly shown. This cracking may be the result of drying or some type of decay in the cedar, as the sample was a piece of a dead branch.

Figure 12. Low-magnification inverted backscatter image of dried cedar. Note the growth rings and the presence of many larger vessels or tracheids.

Figure 13. Higher-magnification inverted backscatter image of the microstructure of dried cedar.

Appendix 1: Properties of Low-melting Bi-Sn Alloys from Alloy Digest by engineering Alloys digest, Inc. [16]

References

[1]Rose, ET and DeRoos, LF, “Infiltration of Metallographic Specimens with Metallic Alloys” in Microstructural Science, 1, Gray, RJ and McCall, JL (eds.), Elsevier, New York, 1974, pp. 275281.Google Scholar
[2]Craze, RC, Pet Trans, AIME 189 (1950) 287293.Google Scholar
[3]Dullien, FAL, Powder Technol 29 (1981) 109116.CrossRefGoogle Scholar
[4]Yadev, GD, Dullian, FAL, Chatzis, I, and Macdonald, IF, “Microscopic Distribution of wetting and Non-Wetting Phases in Sandstone During Immiscible Displacements,” paper 13212 in Proc SPE Annual Technical Conf, Dallas, (1984).Google Scholar
[5]Shultz, RL, Lyons, RG, and Steele, JH, Trans I&SM (1986) 4554.Google Scholar
[6]Steele, JH and Engel, R, Adv Ceram Mater 3 (1988) 452456.CrossRefGoogle Scholar
[7]Nemati, KM, Monteiro, PJM, and Scrivener, KL, Am Concrete Inst Mat J 95 (1998) 617631.Google Scholar
[8]Scrivener, KL and Nemati, KM, Cement Concrete Res 26 (1996) 3540.CrossRefGoogle Scholar
[9]Chang, CT, Monteiro, PJM, Nemati, KM, and Shyu, K, J Mater Civil Eng 8 (1996) 157170.CrossRefGoogle Scholar
[10]Ritter, HL and Drake, LC, Ind & Eng Chem Anal Ed 17 (1945) 782791.CrossRefGoogle Scholar
[11]Xia, Y, Gates, B, Yin, Y, and Lu, Y, Adv Mater 12 (2000) 693713.3.0.CO;2-J>CrossRefGoogle Scholar
[12]Mayoral, R, Requena, J, Lopez, C, Moya, SJ, Miguez, H, Vazquez, L, Meseguer, F, Holgado, M, Cintas, A, and Blanco, A, Adv Mater 9 (1997) 257260.CrossRefGoogle Scholar
[13]Steele, J, Micros Microanal 15 (supp 2) 2009, paper 474.Google Scholar
[14]Steele, JH, Micros Microanal 8 (supp 2) 2002, p. 1262CD.CrossRefGoogle Scholar
[15]Ostyn, KM, Carter, CB, Koehne, M, Falke, H, and Schmalzried, H, J Am Ceram Soc 67(10) (1984) 679685.CrossRefGoogle Scholar
[16]Engineering Alloys Digest, Inc., Alloy Digest, Upper Montclair, NJ, 1975.Google Scholar
Figure 0

Figure 1. Diagram showing the mounting press with O-rings hold the liquid metal under the pressure needed to infiltrate a porous sample.

Figure 1

Figure 2. Photograph of a 1-inch diameter Cerrotru alloy mount of a partially reduced Taconite (Hematite) pellet from Shultz et al. [5].

Figure 2

Figure 3. Fracture surface of 425-nm mono-size silica sphere packing showing 100 type planes and close-packed 111-type planes (from Mayoral et al. [12]).

Figure 3

Figure 4. Backscatter image of 0.5 micron silica sphere packing that has been filled with Bi-Sn alloy. The stacking faults and the grain-like packing of the spherical particles can be observed.

Figure 4

Figure 5. A higher magnification BSE image of a polished section of 0.5 micron silica sphere packing showing filled interstices through the silica particles.

Figure 5

Figure 6. Inverted BS image of pottery shard after filling with Bi-Sn and polishing. Varying gray shades are the result of atomic number contrast.

Figure 6

Figure 7. Higher magnification view of the microstructure of a pottery shard. Note that the clay microstructure consists of two phases that may be the result of incomplete transformation to mullite.

Figure 7

Figure 8. Low-magnification inverted backscatter image of a magnesia-chromite refractory brick. Note: MgO = white, Pores (P) = black, Cr2O3 = light gray, and Fe2O3 = dark gray.

Figure 8

Figure 9. Inverted backscatter image showing chromite interface and spinel precipitates within the MgO phase. The filled pores and cracks that connect them can be readily observed. The scale marker is 0.1 mm.

Figure 9

Figure 10. Higher-magnification backscatter image of MgO regions showing SiO2 layers separating MgO grains that have fine spinel precipitates formed within them.

Figure 10

Figure 11. High-magnification inverted backscatter image showing a silica layer between MgO grains that contain fine spinel precipitates. Argon-ion etching of the mechanically polished surface is required to observe these fine cruciform-shaped spinel precipitates.

Figure 11

Figure 12. Low-magnification inverted backscatter image of dried cedar. Note the growth rings and the presence of many larger vessels or tracheids.

Figure 12

Figure 13. Higher-magnification inverted backscatter image of the microstructure of dried cedar.

Figure 13

Appendix 1: Properties of Low-melting Bi-Sn Alloys from Alloy Digest by engineering Alloys digest, Inc. [16]