Fundamental Properties of Monolithic Bentonite Buffer Material Formed by Cold Isostatic Pressing for High-Level Radioactive Waste Repository

Published online by Cambridge University Press:  10 February 2011

S. Kawakami
Affiliation:
Ishikawajima-Harima Heavy Industries Co., Ltd., Yokohama, Japan
Y Yamanaka
Affiliation:
Ishikawajima-Harima Heavy Industries Co., Ltd., Yokohama, Japan
K. Kato
Affiliation:
Ishikawajima-Harima Heavy Industries Co., Ltd., Yokohama, Japan
H. Asano
Affiliation:
Ishikawajima-Harima Heavy Industries Co., Ltd., Yokohama, Japan
H. Ueda
Affiliation:
Tokyo Electric Power Company, Tokyo, JAPAN.
Get access

Abstract

The methods of fabrication, handling, and emplacement of engineered barriers used in a deep geological repository for high level radioactive waste should be planned as simply as possible from the engineering and economic viewpoints. Therefore, a new concept of a monolithic buffer material around a waste package have been proposed instead of the conventional concept with the use of small blocks, which would decrease the cost for buffer material. The monolithic buffer material is composed of two parts of highly compacted bentonite, a cup type body and a cover. As the forming method of the monolithic buffer material, compaction by the cold isostatic pressing process (CIP) has been employed.

In this study, monolithic bentonite bodies with the diameter of about 333 mm and the height of about 455 mm (corresponding to the approx. 1/5 scale for the Japanese reference concept) were made by the CIP of bentonite powder. The dry densities: pd of the bodies as a whole were measured and the small samples were cut from several locations to investigate the density distribution. The swelling pressure and hydraulic conductivity as function of the monolithic body density for CIP-formed specimens were also measured.

High density ( ρd: 1.4–2.0 Mg/m3) and homogeneous monolithic bodies were formed by the CIP. The measured results of the swelling pressure (3–15 MPa) and hydraulic conductivity (0.5–1.4×10−3 m/s) of the specimens were almost the same as those for the uniaxial compacted bentonite in the literature. It is shown that the vacuum hoist system is an applicable the handling method for emplacement of the monolithic bentonite.

Type
Research Article
Copyright
Copyright © Materials Research Society 1999

Access options

Get access to the full version of this content by using one of the access options below. (Log in options will check for institutional or personal access. Content may require purchase if you do not have access.)

References

REFERENCES

1. Saito, S., Umeda, N., Press technology, 10, 1 (1972).Google Scholar
2. Strijbos, S., Powder Technology, 18, 187 (1977).Google Scholar
3. Mikage, T., Umeda, N., Ceramics, 18–12, 1054 (1983).Google Scholar
4. Power Reactor and Nuclear Fuel Development Corporation, PNC TN 1410 92-081 (1992)Google Scholar
5. SKB (Swedish Nuclear Fuel and Waste Management Co), SKB Technical Report 91-33 (1991)Google Scholar